Yield, Tensile and Shear Strength: What Matters When You Punch and Bend Steel
Last updated: November 2026
You'll hear three strengths when people talk about steel: yield, tensile and shear. They aren't the same thing, and each one matters for a different job. The short answer: punching and shearing follow shear strength, press brake tonnage follows tensile strength, and yield strength mostly shows up as springback. Here's what each one means and how it affects your work.
The three numbers
| Yield strength | Tensile (ultimate) strength | Shear strength | |
|---|---|---|---|
| What it is | The stress where steel starts to bend permanently instead of springing back | The highest stress steel can take before it tears apart when pulled | The stress it takes to cut steel across, the way a punch or shear blade does |
| ASTM A36 minimum | 36,000 psi | 58,000 psi (range 58,000 to 80,000) | Not specified; about 70–80% of tensile |
| A36 plate, typical tested average* | About 47,000 psi | About 68,000 psi | About 48,000–54,000 psi** |
| Matters for | Springback and angle consistency | Press brake tonnage | Punching, shearing and notching tonnage |
*AISC survey of 14,900 mill test reports, plate 3/16" to 3/4" thick. **Estimated at 70–80% of the average tensile strength; mill test reports don't list shear strength.
Yield and shear are easy to mix up because the numbers can look similar on paper, but they measure different things. Yield is where steel starts to bend for good. Shear, like tensile, is a breaking point: it's where the steel gives way and cuts.
Punching: shear strength, which follows tensile
Punching cuts a slug out of the plate, so the force depends on the steel's shear strength. For mild steel, shear strength is about 70 to 80 percent of tensile strength. That's why punch tonnage charts and calculators are built on a shear value, and why stronger plate takes more tonnage even at the same thickness.
Punch tonnage = length of cut (π × diameter for a round hole) × thickness × shear strength ÷ 2,000. Iroquois uses 60,000 psi shear for A36; see the punch tonnage chart.
Bending: tonnage follows tensile, springback follows yield
Press brake tonnage formulas are scaled by tensile strength. The standard approach takes the force for 60,000 psi baseline steel and multiplies it by your material's tensile strength divided by 60,000. Plate that tests at 72,000 psi tensile needs about 20 percent more force than the baseline.
Yield strength shows up differently. The higher the yield, the more the steel springs back after the punch releases. Two pieces of "A36" with different yields can bend to different angles with the same setting, which is one reason a new batch of plate can need its stroke adjusted.
Why press brake work uses two different numbers
Bending involves both yield and tensile strength, because they answer two different questions:
- How hard does the machine have to push? That's tonnage, and the industry standard is to figure it from tensile strength. Bending starts once the steel passes its yield point, but as the bend forms, the steel at the outside of the bend stretches and gets stronger as it's worked. The force the machine has to deliver ends up tracking tensile strength more closely than yield, which is why nearly every press brake chart and formula, including Iroquois charts, is based on tensile.
- How much will the part spring back when the punch lifts? That depends on yield strength. The higher the yield, the more the steel springs back toward flat.
So you size the press brake by tensile strength, and you set your angle expecting springback from yield strength.
Why the ratio matters
A36 has a low yield-to-tensile ratio, averaging about 0.69 in the AISC survey: there's a wide gap between where it starts to bend permanently and where it breaks. That gap is what makes A36 forgiving to form. Higher-strength steels have ratios closer to 0.9, leaving less margin, so they spring back more and generally need larger inside bend radii.
What to use, and when
Most fabricators never see a mill test report for the steel they buy, so in practice you plan for the high end of the range. If you do have the report, use its numbers.
| Job | Number that matters | What to assume for A36 |
|---|---|---|
| Punching, shearing, notching | Shear strength | 60,000 psi shear (what the Iroquois punch chart uses) |
| Press brake tonnage | Tensile strength | 72,000 psi tensile (what the Iroquois press brake chart uses) |
| Springback and angle consistency | Yield strength | Often 45,000 to 55,000 psi, and it can change from one batch of steel to the next |
For why today's A36 tests higher than its name suggests, see A36 vs. Mild Steel Explained.
FAQ
Is shear strength the same as yield strength?
No. Yield strength is where steel starts to bend permanently. Shear strength is the stress it takes to cut steel across, the way a punch or shear blade does. Like tensile strength, it's a breaking point, and for mild steel it's about 70 to 80 percent of tensile strength.
Is punching tonnage based on tensile or yield strength?
Neither directly; it's based on shear strength, which for mild steel is roughly 70 to 80 percent of tensile strength. Yield strength doesn't set punching force.
Is press brake tonnage based on tensile or yield strength?
Bending tonnage charts and formulas are scaled by tensile strength: material factor = tensile strength ÷ 60,000 psi. Yield strength mainly affects springback.
Why does higher-strength steel spring back more?
Springback grows with yield strength. Steel that yields higher, such as dual-certified A36/A572 Grade 50, springs back more after air bending, so you need to bend further past your target angle.
Sources
- R. L. Brockenbrough, "MTR Survey of Plate Material Used in Structural Fabrication," AISC Engineering Journal, 2003
- MetalForming, August 2010: shear strength of mild steel as 70–80% of tensile
- The Fabricator, "Tonnage limits for press brake applications"