A36 vs. Mild Steel Explained
What's the difference, and which chart should I use?
Last updated: November 2026
"Mild steel" and "A36" get used like they mean the same thing, and nearly every punching and press brake tonnage chart is labeled with one or the other. They aren't quite the same. Mild steel is a general name; A36 is a specification that only sets minimums, and the A36 you buy today usually tests much stronger than those minimums and stronger than the "mild steel" many charts assume. Here's the difference and what it means for the chart you use.
The short answer: On most charts, "mild steel" means steel of about 60,000 psi tensile. A36 is a specific grade with a 58,000 to 80,000 psi tensile range, and real A36 plate averages about 68,000 psi tensile and 47,000 psi yield. Use a chart built on the high end of A36, or add about 20 percent to a "mild steel" chart.
What "mild steel" means
Mild steel is a general name for low-carbon steel, not a specification. It welds, cuts, punches and bends easily, which is why it's the everyday steel of fabrication shops. Because there's no single spec behind the name, there's no single strength either. When a tonnage chart says "mild steel," it means whatever baseline the chart maker picked, most often about 60,000 psi tensile.
Most hot-rolled plate and bar is A36. Thinner hot-rolled sheet, under 1/4", is made at the mill to a separate sheet specification (ASTM A1011, formerly A569), and suppliers sell it either as A36 or as commercial steel sheet. Commercial steel sheet is usually the same strength as A36 or a little softer, so a chart built on the high end of A36 covers both.
Where the "36,000 psi mild steel" idea comes from
Before 1960, the basic structural steel in the U.S. was ASTM A7, with a minimum yield of 33,000 psi and a tensile strength of about 60,000 to 72,000 psi. A36 was introduced in 1960 with a 36,000 psi minimum yield and better weldability, and A7 was withdrawn in 1967. So the 36,000 psi number many of us remember as "mild steel" is really A36's own minimum yield, and the 60,000 psi tensile baseline on so many charts matches the steel of that era.
What has changed is how steel is made. Much of today's structural steel is melted from scrap in electric arc furnaces, and scrap carries small amounts of copper, nickel, chromium and other elements that raise strength. Add modern rolling practice and dual certification, and today's A36 tests well above both the old A7 numbers and its own 36,000 psi minimum.
What A36 is
ASTM A36 is the standard specification for carbon structural steel in plate, bar and shapes such as angle and channel. A36 is a mild steel, and if a shop buys "plate" or "flat bar" without naming a grade, it's usually A36. The difference is that A36 comes with a defined range of strengths, and that range reaches well above the typical "mild steel" baseline.
Three ways to measure strength
Steel strength gets described three ways, and each one matters for a different job:
- Yield strength: the point where steel stops springing back and starts to bend permanently. It mostly affects springback.
- Tensile strength: the point where steel tears apart when pulled. Press brake tonnage is figured from it.
- Shear strength: the force it takes to cut steel across, the way a punch or shear blade does. For mild steel it's about 70 to 80 percent of tensile strength. Punching, shearing and notching tonnage are figured from it.
For more on how each one affects your work, see Yield, Tensile and Shear Strength: What Matters When You Punch and Bend Steel.
What the A36 specification guarantees
| Property | ASTM A36 requirement |
|---|---|
| Yield strength | 36,000 psi minimum (32,000 psi for plate over 8" thick) |
| Tensile strength | 58,000 to 80,000 psi |
| Upper limit on yield | None |
| Shear strength | Not specified; about 70–80% of tensile |
The specification sets a floor, not a target. A mill can ship steel much stronger than 36,000 psi yield and still call it A36. That missing upper limit on yield is what makes dual certification possible.
How strong A36 really is: 14,900 mill test reports
The best answer comes from a survey the American Institute of Steel Construction (AISC) sponsored of actual mill test reports, the certificates mills issue with each heat of steel. It covered 14,900 reports for A36 plate 3/16" to 3/4" thick, and was published in AISC's Engineering Journal in 2003.
(spec minimum: 36,000)
(spec range: 58,000–80,000)
A36 plate, 3/16" to 3/4"
Thicker plate (over 3/4" to 4") averaged 43,100 psi yield. Source: R. L. Brockenbrough, AISC Engineering Journal, 2003 (read the report).
Two other sources point the same way:
- Building code: AISC's seismic provisions tell engineers to expect A36 yield at 1.5 times the 36,000 psi minimum (about 54,000 psi) and tensile at 1.2 times the 58,000 psi minimum (about 69,600 psi).
- Dual certification: since the 1990s, mills have commonly certified plate and shapes as both A36 and A572 Grade 50. Engineering guidance written after the 1994 Northridge earthquake noted that A36 often exceeds 50,000 psi yield and that new A36 should be assumed to be the dual grade.
In other words, a piece of "A36" from today's supplier is more likely to behave like Grade 50 than like the 36,000 psi steel the name suggests, and it's well above the 60,000 psi "mild steel" baseline on many charts.
Mild steel, A36 and other common grades side by side
| Steel | Yield strength | Tensile strength | Common use |
|---|---|---|---|
| "Mild steel" on most charts | Not a spec | About 60,000 psi assumed | Chart baseline |
| A36 (spec) | 36,000 psi min | 58,000–80,000 psi | Plate, flat bar, angle, channel |
| A36 (tested average) | About 47,000 psi | About 68,000 psi | AISC survey, plate 3/16"–3/4" |
| A1011 CS Type B (commercial steel sheet) | Not specified; typically about 30,000–49,000 psi | Not specified | Hot-rolled sheet under 1/4" (A1011 SS Grade 36 is the version with a guaranteed 36,000 psi minimum yield) |
| A572 Grade 50 | 50,000 psi min | 65,000 psi min | Plate and shapes where more strength is needed |
| A992 | 50,000–65,000 psi | 65,000 psi min | Wide-flange beams (has largely replaced A36 there) |
Dual-certified A36/A572 Grade 50 meets both specs at once, and fabricators generally pay the same price for it as plain A36.
Which chart should I use?
Check what the chart is based on. Many older charts were built on "mild steel" at about 60,000 psi tensile. For bending, that's the basis of the classic 575 press brake formula. For punching, the common hole diameter × thickness × 80 rule works out to about 51,000 psi shear strength (shear being the force to cut steel across, about 70–80% of tensile). Both sit near the bottom of what A36 actually tests at, so those charts can come up 10 to 20 percent short.
| Job | "Mild steel" chart | A36 at the high end |
|---|---|---|
| Punch a 1" hole in 1/2" plate | 40 tons (about 51,000 psi shear) | 47 tons (60,000 psi shear) |
| Air bend 1/4" plate in a 2" die | 18.0 tons per foot (60,000 psi tensile) | 21.6 tons per foot (72,000 psi tensile) |
- Best: use a chart built on A36 at the high end. Iroquois charts are: the punch tonnage chart uses 60,000 psi shear strength, and the press brake bending chart in our owner's manuals uses 72,000 psi tensile strength with a recommended safety factor of at least 20 percent.
- If your chart says "mild steel" at 60,000 psi: add about 20 percent for A36.
- If you have a mill test report: use its tensile number. Most fabricators never see one, so plan for the high end and leave some headroom when a job is close to your machine's limit.
FAQ
Is A36 the same as mild steel?
A36 is a mild steel, but "mild steel" isn't a specification. It's a general name for low-carbon steel. On tonnage charts, "mild steel" usually means an assumed strength of about 60,000 psi tensile. A36 is a specific ASTM grade, and today's A36 usually tests stronger than that.
Which tonnage chart should I use for A36?
Use a chart built on A36 at the high end of its range, such as the Iroquois charts (60,000 psi shear for punching, 72,000 psi tensile for bending). If your chart is based on 60,000 psi tensile mild steel, multiply its press brake numbers by about 1.2 for A36. For punch charts using the diameter × thickness × 80 rule, multiply by about 1.2 as well. You can also adjust any chart yourself: divide the chart’s tonnage by the tensile strength the chart is based on, then multiply by your material’s tensile strength. For example, if the chart shows 21.6 tons for a bend and is based on 72,000 psi tensile, and your material tests at 80,000 psi tensile: 21.6 ÷ 72,000 × 80,000 = 24 tons.
What is the tensile strength of A36 steel?
The specification requires 58,000 to 80,000 psi tensile strength and a minimum yield strength of 36,000 psi. An AISC survey of 14,900 mill test reports found A36 plate 3/16" to 3/4" thick averaged about 67,900 psi tensile and 46,900 psi yield.
What is the shear strength of A36 steel?
The A36 specification doesn't list shear strength. For mild steel it runs about 70 to 80 percent of tensile strength. Iroquois punch charts use 60,000 psi shear, toward the high end for A36.
What is dual-certified A36/A572 Grade 50?
Steel that meets both specifications at once: A36 (36,000 psi minimum yield) and A572 Grade 50 (50,000 psi minimum yield, 65,000 psi minimum tensile). Mills produce it because one product can be sold as either grade.
Sources
- R. L. Brockenbrough, "MTR Survey of Plate Material Used in Structural Fabrication," AISC Engineering Journal, 2003
- AISC 341, Seismic Provisions for Structural Steel Buildings, Table A3.1 (expected strength ratios Ry and Rt)
- SAC Joint Venture, Interim Guidelines, Chapter 8: Metallurgy and Welding
- The Fabricator, "The 4 pillars of press brake tonnage limits"
- Roper Whitney, punch tonnage reference charts